The Secrets of Battery Runtime
NOTE: This article has been archived. Please read our new "Four Renegades of Battery Failure" for an updated version.
Declining Capacity
Energy storage in a battery can conceptually be divided into three imaginary segments of the available energy,the empty zone that can be refilled, and the unusable part (rock content). Figure 1 illustrates these three sections.
Figure 1: Aging battery
Batteries begin fading from the day they are manufactured.A new battery should deliver 100 percent capacity; most packs in use operate at less.
Courtesy of Cadex
Although the manufacturer specifies the runtime of portable equipment based on a battery performing at 100 percent, most packs in the field operate at less capacity. As time goes on, the performance declines further and the battery gets smaller in terms of holding capacity. A pack should be replaced when the capacity drops to 80 percent. This is only 20 percent down from 100 percent, and the end-of-life threshold may vary according to application and company policy.
Besides age-related losses, sulfation and grid corrosion are the main killers of lead acid batteries. Sulfation is a thin layer that forms on the negative cell plate if the battery is allowed to dwell in a low state-of-charge. If sulfation is caught in time, an equalizing charge can reverse the condition. [BU-804, Sulfation] With nickel-based batteries, the so-called rock content is often the result of crystalline formation, also known as “memory,” and a full discharge can sometimes restore the battery. The aging process of lithium-ion is cell oxidation, a process that occurs naturally as part of usage and aging and cannot be reversed.
Rising Internal Resistance
High capacity has limited use if the battery is unable to deliver the stored energy effectively. To bring the power out, the battery needs low internal resistance. Measured in milliohms (mW), resistance is the gatekeeper of the battery; the lower the value, the less restriction the pack encounters. This is especially important with heavy loads and high current pulses, as elevated resistance causes the voltage to collapse and trigger an earlyshutdown. The device turns off and valuable energy is left behind. Figure 2 illustrates batteries with low and high internal resistance as free-flowing and restricted taps.
|
|
Figure 2: Effects of internal battery resistance A battery with low internal resistance delivers high current on demand. High resistance causes the battery voltage to collapse. The equipment cuts off, leaving energy behind. Courtesy of Cadex |
Lead acid has a very low internal resistance, and the battery responds well to high current bursts lasting for only a few seconds. Due to inherent sluggishness, however, lead acid does not perform well with a sustained discharge at high current and the battery needs rest to recover. Sulfation and grid corrosion are the main causes of increased internal resistance. Temperature also affects the resistance; heat lowers it and cold raises it.
Alkaline, carbon-zinc and other primary batteries have relatively high internal resistance, and this relegates their use to low-current applications such as flashlights, remote controls, portable entertainment devices and kitchen clocks. As the batteries discharge, the resistance increases further. This explains why regular alkaline cells have a relatively short runtime in digital cameras. The high internal resistance limits most primary batteries to “soft” applications, and using them to drive power tools that draw high amperage is unthinkable.
Figures 3, 4 and 5 reflect the talk-time of cellular phones with pulsed discharge loads of 1C, 2C and 3C, which GSM and CDMA demand. All batteries tested are similar in size and have capacities of 113%, 94% and 107% respectively, when checked with a battery analyzer on a DC discharge. The three graphs clearly demonstrate the importance of low internal resistance, which varies from a low 155mΩto a moderate 320mΩ, to a high 778mΩ respectively.
Figure 3: GSM discharge pulses at 1, 2, and 3C with resulting talk-time
The capacity of the NiCd battery is 113%; the internal resistance is 155mΩ.
Figure 4: GSM discharge pulses at 1, 2, and 3C with resulting talk-time
The capacity of the NiMH battery is 94%, the internal resistance is 320mΩ.
Figure 5: GSM discharge pulses at 1, 2, and 3C with resulting talk-time
The capacity of the Li-ion battery is 107%; the internal resistance is 778mΩ.
All three figures courtesy of Cadex
Notes: The above tests were done on cellular phone batteries before lithium-ion took over as the leading battery type for this application. The internal resistance of a modern cellular battery is between 150 and 350mΩ.
The maximum discharge pulse current of GSM is 2.5 amperes. When drawn from an 800mAh pack, this represents a 3C discharge, or three times the rated current.
Elevated Self-discharge
All batteries are affected by self-discharge. Self-discharge is not a manufacturing defect per se, although poor manufacturing practices and improper handling can promote the problem. The amount of electrical leakage varies with chemistry, and primary cells, such as lithium and alkaline, are among the best in retaining the energy. Nickel-based rechargeable systems, in comparison, leak the most and need recharging if the battery has not been used for a few days. High-performance nickel-based batteries are subject to higher self-discharge than the standard versions with lower energy densities. Figure 6 illustrates in the form of leaking fluids the self-discharge of a battery.
Figure 6: Effects of high self-discharge
Self-discharge increases with age, cycling and elevated temperature. Discard a battery if the self-discharge reaches 30 percent in 24 hours.
Courtesy of Cadex
One of the best batteries in terms of self-discharge is lead acid; it loses only five percent per month. This chemistry also has the lowest specific energy and is ill suited for portable use. Lithium-ion self-discharges about five percent in the first 24 hours and 1 to 2 percent thereafter. The need for the protection circuit increases the discharge by another three percent per month.
The self-discharge on all battery chemistries increases at higher temperatures and the rate typically doubles with every 10°C (18°F). A noticeable energy loss occurs if a battery is left in a hot vehicle. Cycling and aging also increase self-discharge. Nickel-metal-hydride is good for 300-400 cycles, whereas the standard nickel-cadmium lasts over 1,000 cycles before elevated self-discharge starts interfering with performance. The self-discharge on an older nickel-based battery can get so bad that the pack loses its energy mainly through leakage rather than normal use during the day. Discard a battery if the self-discharge reaches 30 percent in 24 hours.
The self-discharge of Li-ion is reasonably steady throughout the service life and does not increase noticeably with age, unless there is a cell anomaly caused by separator damage when microscopic metal particles group together. Improved manufacturing methods have minimized this problem on newer batteries.Table 8 reveals the self-discharge rate per month at various temperatures and state-of-charge conditions.
Charge condition | 0°C (32°F) | 25°C (77°F) | 60°C (140°F) |
Full charge 40–60% charge | 6% 2% | 20% 4% | 35% 15% |
Table 8: Self-discharge of Li-ion at various temperatures and state-of-charge
Self-discharge increases with rising temperature and higher SoC.
Once present, the high self-discharge of a flooded lead acid battery cannot be reversed. Factors leading to this failure are sludge buildup in the sediment trap on the bottom of the container. The sludge is semi-conductive, and when substance reaches to the plates a soft short occurs. On nickel-based batteries, a weakened or damaged separator is the cause of high self-discharge. Contributing factors are crystalline formation (memory), permitting the battery to “cook” in the charger or exposing it to repeated deep discharge cycles. A faulty separator also increases the self-discharge in lithium-ion batteries. In extreme cases, heat generated by the electrical leak further weakens the damaged separator. This can lead to a thermal breakdown.
Premature Voltage Cut-off
Not all stored battery energy can or should be used on discharge, and some reserve is almost always left behind when the equipment cuts off. There are several reasons for this.
Most cell phones, laptops and other portable devices turn off when the lithium-ion battery reaches 3V/cell on discharge. The manufacturers choose this relatively high voltage threshold to allow for some self-discharge while in storage, giving a grace period before the protection circuit opens at about 2.5V/cell.
A hybrid battery on a car never fully discharges and operates on a state-of-charge of 20 to 80 percent. This is the most effective working bandwidth of the battery, and staying within this range delivers the longest service life. A deep discharge with a full recharge causes undue stress to any battery, including Li-ion. Nickel-based batteries are similar, and because of reduced charge acceptance and heat buildup above the 80 percent SoC, the batteries are seldom fully charged. The emphasis on an electric powertrain is on maximizing service life rather than optimizing runtime (as is the case with consumer products).
Power tools and medical devices that draw high currents push the battery voltage to an early cut-off. This is especially true if one of the cells has a high internal resistance, or when the battery is operating at cold temperatures. These batteries may still have ample capacity left after the “cut-off” and when discharging at moderate load, a battery analyzer may read a residual capacity of 30 percent. Figure 9 illustrates the cut-off voltage graphically.
Figure 9: Illustration of equipment with high cut-off voltage
Portable devices do not utilize all available battery power and leave some energy behind.
Courtesy of Cadex
Last Updated: 5-Jul-2016
Batteries In A Portable World
The material on Battery University is based on the indispensable new 4th edition of "Batteries in a Portable World - A Handbook on Rechargeable Batteries for Non-Engineers" which is available for order through Amazon.com.
Find An Article
Table of Contents
-
Introduction 4>
- BU-001: Sharing Battery Knowledge
- BU-002: Introduction
- BU-003: Dedication
-
Crash Course on Batteries 4>
- BU-101: When Was the Battery Invented?
- BU-102: Early Innovators
- BU-103: Global Battery Markets
- BU-103a: Battery Breakthroughs: Myth or Fact?
- BU-104: Getting to Know the Battery
- BU-104a: Comparing the Battery with Other Power Sources
- BU-104b: Battery Building Blocks
- BU-104c: The Octagon Battery – What makes a Battery a Battery
- BU-105: Battery Definitions and what they mean
- BU-106: Advantages of Primary Batteries
- BU-106a: Choices of Primary Batteries
- BU-107: Comparison Table of Secondary Batteries
-
Battery Types 4>
- BU-201: How does the Lead Acid Battery Work?
- BU-201a: Absorbent Glass Mat (AGM)
- BU-201b: Gel Lead Acid Battery
- BU-202: New Lead Acid Systems
- BU-203: Nickel-based Batteries
- BU-204: How do Lithium Batteries Work?
- BU-205: Types of Lithium-ion
- BU-206: Lithium-polymer: Substance or Hype?
- BU-208: Cycling Performance
- BU-209: How does a Supercapacitor Work?
- BU-210: How does the Fuel Cell Work?
- BU-210a: Why does Sodium-sulfur need to be heated
- BU-210b: How does the Flow Battery Work?
- BU-211: Alternate Battery Systems
- BU-212: Future Batteries
- BU-214: Summary Table of Lead-based Batteries
- BU-215: Summary Table of Nickel-based Batteries
- BU-216: Summary Table of Lithium-based Batteries
- BU-217: Summary Table of Alternate Batteries
- BU-218: Summary Table of Future Batteries
-
Packaging and Safety 4>
- BU-301: A look at Old and New Battery Packaging
- BU-301a: Types of Battery Cells
- BU-302: Series and Parallel Battery Configurations
- BU-303: Confusion with Voltages
- BU-304: Why are Protection Circuits Needed?
- BU-304a: Safety Concerns with Li-ion
- BU-304b: Making Lithium-ion Safe
- BU-304c: Battery Safety in Public
- BU-305: Building a Lithium-ion Pack
- BU-306: What is the Function of the Separator?
- BU-307: How does Electrolyte Work?
- BU-308: Availability of Lithium
- BU-309: How does Graphite Work in Li-ion?
- BU-310: How does Cobalt Work in Li-ion?
- BU-311: Battery Raw Materials
-
Charge Methods 4>
- BU-401: How do Battery Chargers Work?
- BU-401a: Fast and Ultra-fast Chargers
- BU-402: What Is C-rate?
- BU-403: Charging Lead Acid
- BU-404: What is Equalizing Charge?
- BU-405: Charging with a Power Supply
- BU-406: Battery as a Buffer
- BU-407: Charging Nickel-cadmium
- BU-408: Charging Nickel-metal-hydride
- BU-409: Charging Lithium-ion
- BU-409a: Why do Old Li-ion Batteries Take Long to Charge?
- BU-409b: Charging Lithium Iron Phosphate
- BU-410: Charging at High and Low Temperatures
- BU-411: Charging from a USB Port
- BU-412: Charging without Wires
- BU-413: Charging with Solar, Turbine
- BU-413a: How to Store Renewable Energy in a Battery
- BU-414: How do Charger Chips Work?
- BU-415: How to Charge and When to Charge?
-
Discharge Methods 4>
- BU-501: Basics about Discharging
- BU-501a: Discharge Characteristics of Li-ion
- BU-502: Discharging at High and Low Temperatures
- BU-503: Determining Power Deliver by the Ragone Plot
- BU-504: How to Verify Sufficient Battery Capacity
-
"Smart" Battery 4>
- BU-601: How does a Smart Battery Work?
- BU-602: How does a Battery Fuel Gauge Work?
- BU-603: How to Calibrate a “Smart” Battery
- BU-603a: Calibrating SMBus Batteries with Impedance Tracking
- BU-604: How to Process Data from a “Smart” Battery
- BU-605: Testing and Calibrating Smart Batteries
-
From Birth to Retirement 4>
- BU-701: How to Prime Batteries
- BU-702: How to Store Batteries
- BU-703: Health Concerns with Batteries
- BU-704: How to Transport Batteries
- BU-704a: Shipping Lithium-based Batteries by Air
- BU-704b: CAUTION & Overpack Labels
- BU-704c: Class 9 Label
- BU-704d: NFPA 704 Rating
- BU-704e: Battery for Personal and Fleet Use
- BU-705: How to Recycle Batteries
- BU-705a: Battery Recycling as a Business
- BU-706: Summary of Do's and Don'ts
-
How To Prolong Battery Life 4>
-
General 4>
- BU-801: Setting Battery Performance Standards
- BU-801a: How to Rate Battery Runtime
- BU-801b: How to Define Battery Life
- BU-802: What Causes Capacity Loss?
- BU-802a: How does Rising Internal Resistance affect Performance?
- BU-802b: What does Elevated Self-discharge Do?
- BU-802c: How Low can a Battery be Discharged?
- BU-803: Can Batteries Be Restored?
- BU-803a: Cell Matching and Balancing
- BU-803b: What causes Cells to Short?
- BU-803c: Loss of Electrolyte
-
Lead Acid 4>
- BU-804: How to Prolong Lead-acid Batteries
- BU-804a: Corrosion, Shedding and Internal Short
- BU-804b: Sulfation and How to Prevent it
- BU-804c: Acid Stratification and Surface Charge
- BU-805: Additives to Boost Flooded Lead Acid
- BU-806: Tracking Battery Capacity and Resistance as part of Aging
- BU-806a: How Heat and Loading affect Battery Life
-
Nickel-based 4>
- BU-807: How to Restore Nickel-based Batteries
- BU-807a: Effect of Zapping
-
Lithium-ion 4>
- BU-808: How to Prolong Lithium-based Batteries
- BU-808a: How to Awaken a Sleeping Li-ion
- BU-808b: What Causes Li-ion to Die?
- BU-808c: Coulombic and Energy Efficiency with the Battery
- BU-809: How to Maximize Runtime
- BU-810: What Everyone Should Know About Aftermarket Batteries
- BU-811: Assuring Minimum Operational Reserve Energy (MORE)
-
Battery Testing and Monitoring 4>
- BU-901: Fundamentals in Battery Testing
- BU-901b: How to Measure the Remaining Useful Life of a Battery
- BU-902: How to Measure Internal Resistance
- BU-902a: How to Measure CCA
- BU-903: How to Measure State-of-charge
- BU-904: How to Measure Capacity
- BU-905: Testing Lead Acid Batteries
- BU-905a: Testing Starter Batteries in Vehicles
- BU-905b: Knowing when to Replace a Starter Battery
- BU-906: Testing Nickel-based Batteries
- BU-907: Testing Lithium-based Batteries
- BU-907a: Battery Rapid-test Methods
- BU-907b: Advancements in Battery Testing
- BU-907c: Cloud Analytics in Batteries
- BU-908: Battery Management System (BMS)
- BU-909: Battery Test Equipment
- BU-910: How to Repair a Battery Pack
- BU-911: How to Repair a Laptop Battery
- BU-915: Testing Battery with EIS
- BU-916: Deep Battery Diagnostics
- BU-917: In Search for Performance Transparency with Batteries
- BU-918: Battery Endurance Plan
- BU-919: Building a Matrix to test Batteries
- BU-920: Matrix Library
- BU-921: Testing Batteries by Multi-Model EIS
- BU-922: What Causes Starter Batteries to Fail?
- BU-923: Getting Deep Cycle Batteries Mission Ready
- BU-924: Battery Ecosystem
- BU-926: Battery Diagnostics, an Overlooked Requirement
-
Amazing Value of a Battery 4>
- BU-1001: Batteries in Industries
- BU-1002: Electric Powertrain, then and now
- BU-1002a: Hybrid Electric Vehicles and the Battery
- BU-1002b: Environmental Benefit of the Electric Powertrain
- BU-1003: Electric Vehicle (EV)
- BU-1003a: Battery Aging in an Electric Vehicle (EV)
- BU-1004: Charging an Electric Vehicle
- BU-1005: Does the Fuel Cell-powered Vehicle have a Future?
- BU-1006: Cost of Mobile and Renewable Power
- BU-1007: Net Calorific Value
- BU-1008: Working towards Sustainability
- BU-1009: Battery Paradox - Afterword
-
Information 4>
- BU-1101: Glossary
- BU-1102: Abbreviations
- BU-1103: Bibliography
- BU-1104: About the Author
- BU-1105: About Cadex (Sponsor)
- BU-1106: Author's Creed
- BU-1107: Disclaimer
- BU-1108: Copyright
-
Learning Tools 4>
- BU-1501 Battery History
- BU-1502 Basics about Batteries
- BU-1504 Battery Test and Analyzing Devices
- BU-1505 Short History of Cadex
-
Battery Articles 4>
- Perception of a Battery Tester
- Green Deal
- Risk Management in Batteries
- Predictive Test Methods for Starter Batteries
- Why Mobile Phone Batteries do not last as long as an EV Battery
- Battery Rapid-test Methods
- How to Charge Li-ion with a Parasitic Load
- Ultra-fast Charging
- Assuring Safety of Lithium-ion in the Workforce
- Diagnostic Battery Management
- Tweaking the Mobile Phone Battery
- Battery Test Methods
- Battery Testing and Safety
- How to Make Battery Performance Transparent
- Battery Diagnostics On-the-fly
- Making Battery State-of-health Transparent
- Batteries will eventually die, but when and how?
- Why does Pokémon Go rob so much Battery Power?
- How to Care for the Battery
- Tesla’s iPhone Moment — How the Powerwall will Change Global Energy Use
- Painting the Battery Green by giving it a Second Life
- Charging without Wires — A Solution or Laziness
- What everyone should know about Battery Chargers
- A Look at Cell Formats and how to Build a good Battery
- Battery Breakthroughs — Myth or Fact?
- Rapid-test Methods that No Longer Work
- Shipping Lithium-based Batteries by Air
- How to make Batteries more Reliable and Longer Lasting
- What causes Lithium-ion to die?
- Safety of Lithium-ion Batteries
- Recognizing Battery Capacity as the Missing Link
- Managing Batteries for Warehouse Logistics
- Caring for your Starter Battery
- Giving Batteries a Second Life
- How to Make Batteries in Medical Devices More Reliable
- Possible Solutions for the Battery Problem on the Boeing 787
- Impedance Spectroscopy Checks Battery Capacity in 15 Seconds
- How to Improve the Battery Fuel Gauge
- Examining Loading Characteristics on Primary and Secondary Batteries
-
Language Pool 4>
- BU-001: Compartir conocimiento sobre baterías
- BU-002: Introducción
- BU-003: Dedicatoria
- BU-104: Conociendo la Batería
- BU-302: Configuraciones de Baterías en Serie y Paralelo
-
Batteries in a Portable World book 4>
- Change-log of “Batteries in a Portable World,” 4th edition: Chapters 1 - 3
- Change-log of “Batteries in a Portable World,” 4th edition: Chapters 4 - 10