How
to restore and prolong lead-acid batteries
The sealed lead acid battery is designed with a low over-voltage potential
to prohibit the battery from reaching its gas-generating state during
charge. This prevents water depletion of the sealed system. Consequently,
these batteries will never get fully charged and some sulfation will develop
over time.
Finding the ideal charge voltage threshold is critical and any level is
a compromise. A voltage limit above 2.40 volts per cell produces good
battery performance but shortens the service life due to grid corrosion
on the positive plate. The corrosion is permanent. A voltage below the
2.40V/cell threshold strains the battery less but the capacity is low
and sulfation sets in over time on the negative plate.
Driven by diverse applications, two sealed lead-acid types have emerged.
They are the sealed lead acid (SLA), and the valve regulated lead acid
(VRLA). Technically, both batteries are the same. Engineers may argue
that the word 'sealed lead acid' is a misnomer because no lead acid battery
can be totally sealed.
The SLA has a typical capacity range of 0.2Ah to 30Ah and powers personal
UPS units, local emergency lighting and wheelchairs. The VRLA battery
is used for large stationary applications for power backup. We are looking
at methods to restore and prolong these two battery systems separately.
The sealed
lead-acid (SLA)
SLA batteries with mild sulfation can be restored but the work is time
consuming and the results are mixed. Reasonably good results are achieved
by applying a charge on top of a charge. This is done by fully charging
an SLA battery, then removing it for a 24 to 48 hour rest period and applying
a charge again The process is repeated several times and the capacity
is checked with a final full discharge and recharge.
Another method of improving performance is by applying an equalizing charge,
in which the charge voltage threshold is increased by about 100mV, typically
from 2.40V to 2.50V. This procedure should last no longer than one to
two hours and must be carried out at moderate room temperature. A careless
equalize charge could cause the cells to heat up and induce venting due
to excessive pressure. Observe the battery during the service.
The cylindrical SLA, made by Hawker and sold under the Cyclone name, requires
slightly higher voltages to reverse sulfation. An adjustable power supply
works best for the service. Set the current limit to the lowest practical
setting and observe the battery voltage and temperature during charge.
Initially, the cell voltage may rise to 5V, absorbing only a small amount
of current. In about two hours, the small charging current converts the
large sulfate crystals back into active material. The internal cell resistance
decreases and the cell starts to clamp the voltage. At around 2.30V, the
cell accepts charge. If the sulfation is advanced, this remedy does not
work and the cell needs replacing.
Sealed lead-acid batteries are commonly rated at a 20-hour discharge.
Even at such a slow rate, a capacity of 100% is difficult to achieve.
For practical reasons, most battery analyzers use a 5-hour discharge when
servicing these batteries. This produces 80% to 90% of the rated capacity.
SLA batteries are normally overrated and manufacturers are aware of this
practice.
Cycling an SLA on a battery analyzer may provide capacity readings that
decrease with each additional cycle. A battery may start off at a marginal
88%, then go to 86%, 84% and 83%. This phenomenon can be corrected by
increasing the charge voltage threshold from 2.40V to 2.45V and perhaps
even 2.50V. Always consider the manufacturer's recommended settings. Cyclone
batteries require slightly higher voltage settings than the plastic version.
Avoid setting the charge voltage threshold too high. In an extreme case,
the limiting voltage may never be reached, especially when charging at
elevated temperatures. The battery continues charging at full current
and the pack gets hot. Heat lowers the battery voltage and works against
a further voltage raise. If no temperature sensing is available to terminate
the charge, a thermal runaway can be the result.
The recovery rate of SLA batteries is a low 15%. Other than reverse sulfation,
there is little one can do to improve SLA. Because the SLA has a relatively
short cycle life, many fail due to wear-out.
Valve
regulated lead-acid (VRLA)
The charge voltage setting on VRLA is generally lower than SLA. Heat is
a killer of VRLA. Many stationary batteries are kept in shelters with
no air conditioning. Every 8°C (15°F) rise in temperature cuts
the battery life in half. A VRLA battery, which would last for 10 years
at 25°C (77°F), will only be good for 5 years if operated at 33°C
(95°F). Once damaged by heat, no remedy exists to improve capacity.
The cell voltages of a VRLA battery must be harmonized as close as possible.
Applying an equalizing charge every 6 months brings all cells to similar
voltage levels. This is done by increasing the cell voltage to 2.50V/cell
for about 2 hours. During the service, the battery must be kept cool and
careful observation is needed. Limit cell venting. Most VRLA vent at 0.3
Bar (5 psi). Not only does escaping hydrogen deplete the electrolyte,
it is highly flammable.
Water permeation, or loss of electrolyte, is a concern with sealed lead
acid batteries. Adding water may help to restore capacity but a long-term
fix is uncertain. The battery becomes unreliable and requires high maintenance.
Simple Guidelines
· Always store lead acid in a charged condition. Never let the
open cell voltage drop much below 2.10V. Apply a topping charge every
six months or when recommended.
· Avoid repeated deep discharges. Charge more often or use a larger
battery.
· Prevent sulfation and grid corrosion by choosing the correct
charge and float voltages.
· Avoid operating Lead-acid at elevated ambient temperatures.
About the Author
Isidor Buchmann is the founder and CEO of Cadex Electronics Inc., in Vancouver
BC. Mr. Buchmann has a background in radio communications and has studied
the behavior of rechargeable batteries in practical, everyday applications
for two decades. Award winning author of many articles and books on batteries,
Mr. Buchmann has delivered technical papers around the world.
Cadex Electronics is a manufacturer of advanced battery chargers, battery
analyzers and PC software. For product information please visit www.cadex.com.
|